Hi!
This is what I do.
My kiln is right beside me as I torch.

I ramp my kiln up to 960 as fast as is healthy for my kiln (some say top speed stresses the kiln out, some say it doesn't... I just do it fast enough to get there within the hour)

Hold for as long as you want to torch, plus 30 mins or so.
I set it to ramp down to 840 at 100 degrees/hr.
I set it to hold for about 45 mins, (some do for much less, but i like to be double darn sure of annealing, and this covers any 'larger' pieces I may make)
After that, how slow you ramp down is up to you....I kinda forget what my kiln is programmed to do, I think it stops at 500 again for 20 mins, and then goes down to 200 and shuts off. It takes mine all night, i don't mind going slow.


Torch! When you deem your bead as "DONE" (large or small) --place it into the kiln.
Keep it up!

When your kiln is down to the last 30 mins, you're done.