First of all, do not try this without good ventilation!! If you dont have a hood and at least 350 cfm fan (or more) with make up air, dont even think about fuming.This will work with all torches from a minor up. ( I have never tried it on a one gas torch. Silver might work, but gold has to have a lot of heat to fume)
Fuming Silver and gold, The basics
First start with pure metals (.999 if possible) I use 1 oz silver ingot from jewelry store. For gold, I found a piece 8 inch's long of 24 karat fine chain at same jeweler.( make sure it's 24 karat. (gold needs to be as pure as possible to fume well)
Prepare a 12 to 14 inch 6-8 mm rod by warming up very end and putting a small dent in top side. ( I use quartz, but boro will work)
Take silver with tweezers, heat up 1/4 inch of ingot. Using glass shears, cut a 2-3 mm strip from ingot. Set aside to cool. Once cool, cut a piece off strip about the size of one half of a BB. (about 2 x 2 mm). Silver strip should cut OK when cool.
For gold, I cut 3-5 links off chain.(very fine chain)
Now, pick up the rod you prepared, using tweezers, put the BB of silver (links of gold) into the dent you made on the rod. Heat up end of rod till till metal melt into small ball. This should hold metal to rod.
Let's fume! Warm piece to be fumed till it has slight glow. Keep turning in last third of flame.
Silver: Place end of rod with silver on top near the end of the "candle" of the flame. When it warms up to the point that it begins to sparkle, you are fuming! Keep piece turning, and "bounce" the end of the rod in and out of the flame. Sliver fumes at a med temp, so you have to keep cooling and reheating fairly fast to keep the process going. You will see the honey yellow color start to appear on you piece. The longer you fume, the darker the color will become, until it turns white. Once you like the color, bring the piece into the working area of the flame, and melt in the fume. Some silver will burn back off, thats normal. you will get the hang of how much to put on for the desired end result. Or you can encase it right away. ( makes a cool effect)
Gold: takes a lot more heat to fume! using a forceful tight flame, begin as with the silver. Once piece is warm, bring the gold into the very tip of a candle (should just touch the end of cone)Leave it there. When The gold starts to "dance" around on the rod you should see color start to show on your piece. (great purple!) the gold has to stay in the cone to fume. ( no bounce like with silver) Again, the longer you fume the darker and richer the color. You can go all the way to gold plate. Melt in as before. Gold does not burn off like silver, so WYSIWYG.
For fun, put dots of clear close(2-3 mm apart) together all over the piece. melt in really well. When you melt it into a ball, it gives a neat honeycomb effect.
__________________
Working with a Red Rocket,Red Max,Natty hand torch-- and tanked oxy from a Homefill system
Bryan M To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2006-01-09, 9:52am
|
|
ManBearPig
|
|
Join Date: Jun 28, 2005
Location: Roanoke, VA
Posts: 8,540
|
|
I have noticed that 22k gold works better than 24k. The impurities in the gold help it stick to the glass. Plus, it doesn't seem to take as much fume with 22k to get the same effects you do with 24k.
And, a hot reducing flame will burn off gold, just like an oxidizing flame burns off silver. So, you have to be careful using both in the same piece. The flame that you use to fume one kind of metal burns off the other kind.
__________________
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2006-01-09, 10:24am
|
|
Formerly SirWatson
|
|
Join Date: Aug 29, 2005
Location: St. Louis, MO
Posts: 1,985
|
|
Can you fume using gold/silver foil or leaf? I see a lot of tutorials talking about fuming with chunks of metal. Since a little metal lasts a long time, I was wondering if the leaf and foil I have will work. I have 22k gold leaf and wanted to try fuming this week. If you can use leaf or foil...what's the best way to use it? Can I ball up the sheet and stick it to the end of my fuming rod, or should I wrap the end of the rod in the sheet and burnish it. Any thoughts?
Thanks!
__________________
Karla Repperger
Studio Solana
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. <><
|
2006-01-09, 10:28am
|
|
ManBearPig
|
|
Join Date: Jun 28, 2005
Location: Roanoke, VA
Posts: 8,540
|
|
You should be able to fume with the leaf. I would ball it up really tightly before picking it up with the rod. You will still lose some it to burn off.
__________________
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2006-01-09, 10:31am
|
|
Retired to the flame
|
|
Join Date: Jan 05, 2006
Location: Central Illinois
Posts: 248
|
|
I have never tried using foil. I don't see why it would not work.I would try the balling up method. The metal starts to melt and trying to move before it starts to fume, so I fear it would fall off the rod with the wrap and burnish method. If you decide to try, let us know how it worked out!!
__________________
Working with a Red Rocket,Red Max,Natty hand torch-- and tanked oxy from a Homefill system
Bryan M To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2006-01-09, 10:32am
|
|
Retired to the flame
|
|
Join Date: Jan 05, 2006
Location: Central Illinois
Posts: 248
|
|
Sorry Chad, must have been typing at the same time!
__________________
Working with a Red Rocket,Red Max,Natty hand torch-- and tanked oxy from a Homefill system
Bryan M To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2006-01-11, 8:43am
|
|
Cheeky & Impervious
|
|
Join Date: Jun 13, 2005
Location: Alabama
Posts: 2,414
|
|
Aside from good ventilation, aren't you supposed to wear a respirator? What rating respirator, will the N100 work?
__________________
~ Jules
He that makes himself a sheep, shall be eaten by the wolves.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2006-01-11, 9:11am
|
|
ManBearPig
|
|
Join Date: Jun 28, 2005
Location: Roanoke, VA
Posts: 8,540
|
|
I guess technically you should. I just sort of hold my breath and lean back a little when I'm fuming. My ventilation is pretty good...
__________________
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2006-01-23, 9:12am
|
|
Member of the Booger7
|
|
Join Date: Sep 19, 2005
Location: Laura, IL - Heard of it? Didn't think so...
Posts: 2,041
|
|
Question
I tried fuming for the first time last night. I made a simple bead using transparent dark aqua then added stacked dots in black and some handmade purple. I ended with black dots. Then I fumed, it turned out neat, but why did the silver only show up on the last black dot? It was all melted flat prior to fuming. Are there certain colors that don't take to fuming or what?
Thanks.
__________________
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. Dianna - To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2006-01-23, 9:20am
|
|
ManBearPig
|
|
Join Date: Jun 28, 2005
Location: Roanoke, VA
Posts: 8,540
|
|
If the glass is too cool (which is what may have happened since you did a lot of work to it) the fume won't stick.
__________________
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. • To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2006-01-23, 10:00am
|
|
Member of the Booger7
|
|
Join Date: Sep 19, 2005
Location: Laura, IL - Heard of it? Didn't think so...
Posts: 2,041
|
|
I see. It actually looked pretty cool, but I just figured I did something weird. Thanks for the tip.
__________________
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. Dianna - To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2006-04-18, 8:51am
|
Junior Member
|
|
Join Date: Apr 18, 2006
Posts: 1
|
|
for me, silver sticks the best when the glass is cool but you need to get it glowing before you throw gold on...i usually do silver and then gold...
|
2007-01-17, 5:52am
|
Senior Member
|
|
Join Date: Dec 22, 2006
Posts: 771
|
|
[quote=firefreak;272254]
Fuming Silver and gold, The basics
Prepare a 12 to 14 inch 6-8 mm rod by warming up very end and putting a small dent in top side. ( I use quartz, but boro will work)
Hello, I was wondering, since some of us only work in soft glass is there another way to introduce the silver to the flame instead of using quartz or boro?
Silver: Place end of rod with silver on top near the end of the "candle" of the flame. When it warms up to the point that it begins to sparkle, you are fuming! Keep piece turning, and "bounce" the end of the rod in and out of the flame.
Here I was wondering if you are actually putting the end of the glass rod into the flame or are you holding slightly below so that the flame is mostly hitting the silver only? Thank you so much for sharing, LeighQUOTE]
|
2007-01-18, 7:45am
|
|
Retired to the flame
|
|
Join Date: Jan 05, 2006
Location: Central Illinois
Posts: 248
|
|
I don't know if you could use a soft glass rod. I will grab a piece of my DW's clear and try later today. i work boro, so quartz works better for me. You have to leave the tip of the rod in the edge of the flame for a while. The boro gets soft and droopy after a few uses. Quartz doesn't.
I don't think there is any way to fume without using a rod. i tried it with a piece of graphite and a little dent at the end. The metal would not stick. It just blew off the rod every time. The idea is to use a rod that takes more heat than the glass your working with.
You want the flame to hit the silver. you don't need much if any of the rod in the flame.
If you need a small piece of boro to use for fuming, Send me your address in a PM and I will send you one.
__________________
Working with a Red Rocket,Red Max,Natty hand torch-- and tanked oxy from a Homefill system
Bryan M To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2009-05-08, 6:41am
|
Cali4nia baby
|
|
Join Date: Aug 22, 2008
Posts: 205
|
|
I read that you can actually do fuming with some of the silver glass rods too ! I must find that info .....arghhhh
|
2009-07-08, 6:46am
|
|
Senior Member
|
|
Join Date: Jul 15, 2005
Location: Eastern West Virginia
Posts: 2,936
|
|
I have not done any fuming for a while - doesn't silver fuming work better in a slightly reducing flame, or am I confused?
__________________
Carol O. (Cricket with 5 lpm oxycon)
"The miracle isn't that I finished. The miracle is that I had the courage to start" John Bingham
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2009-07-08, 7:42am
|
|
Who me?
|
|
Join Date: Jun 15, 2005
Location: Hagerstown, Indiana
Posts: 2,284
|
|
Quote:
Originally Posted by FairyVerre
I read that you can actually do fuming with some of the silver glass rods too ! I must find that info .....arghhhh
|
I've done some gold fuming using rubino.
I just placed some quartz rods to hold your silver and gold in the flame in the garage for sale for those interested. I had little succes trying ot use boro.
__________________
From the Perimeter of the Great Dismal Swamp
|
2010-12-21, 5:14pm
|
Member
|
|
Join Date: Jul 12, 2007
Location: Brooklyn, NY
Posts: 153
|
|
Okay, this is totally awesome. Two questions:
1. Can you fume with a hothead? (Siiigh...)
2. Where can one get the quartz rod set-up for fuming nowadays?
__________________
BE on a hothead with mapp gas
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2010-12-21, 10:34pm
|
|
Formerly FishBulb
|
|
Join Date: Dec 05, 2008
Location: Pony Flower Princess Land
Posts: 2,772
|
|
Hey, this thread is exactly what I've been looking for! I've searched for fuming but this thread never came up, or if it did it was so far near the bottom of the search that I overlooked it. Thank you to everybody who contributed!
__________________
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts. To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
In Soviet Russia, Google searches you.
|
2010-12-21, 10:47pm
|
|
Retired to the flame
|
|
Join Date: Jan 05, 2006
Location: Central Illinois
Posts: 248
|
|
You should be able to fume silver with a hot head. I doubt if you could get the necessary heat or flame environment for gold. Silver likes a reducing flame.
Quartz rod: http://www.dichroicimagery.com/advan...sort=4a&page=2
I use a 12 inch piece of 7mm.
__________________
Working with a Red Rocket,Red Max,Natty hand torch-- and tanked oxy from a Homefill system
Bryan M To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2010-12-22, 7:04am
|
Member
|
|
Join Date: Jul 12, 2007
Location: Brooklyn, NY
Posts: 153
|
|
Oh, sweet, thanks! Though if I'm understanding the instructions right, you need to melt a dent into the rod, and my hothead will never get hot enough to let me do that. Is anyone selling pre-dented rods?
__________________
BE on a hothead with mapp gas
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2010-12-22, 11:09pm
|
|
Retired to the flame
|
|
Join Date: Jan 05, 2006
Location: Central Illinois
Posts: 248
|
|
I don't think you would be able to get the quartz hot enough with a hot head. It took about 5 min if my pre-mix flame to get a 7mm quartz rod hot enough to put a small dent on the end. No one sells a pre-dented rod. For use in a hot head, i would think that a piece of boro rod would work just fine.
The dent on the end of the rod makes it easier to keep the little ball of silver from falling off in the flame. Once the silver starts to warm up, it will sometimes try to "move" around the rod. Or fall off. Once you have fumed with the rod a few times there will be a deposit of silver on the end of the rod that will hold on to the silver just fine. The dent just helps hold the little ball for the first few times.
You don't have to have a special rod to be able to fume. You can use any rod to hold the silver. If you take the color that takes the longest time to melt in your flame, it will work enough to find out what fuming is all about. When you start fuming on a regular basis or for longer amounts of time, then you need a rod that does not melt well in your flame.
__________________
Working with a Red Rocket,Red Max,Natty hand torch-- and tanked oxy from a Homefill system
Bryan M To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
2013-01-19, 10:23pm
|
|
kiwi ( new zealand)
|
|
Join Date: Jun 14, 2010
Location: Wanganui New Zealand
Posts: 240
|
|
thanks for this info firefreak it will help a lot i just got a fume hood and a 650 cmf fan
|
2018-01-30, 4:42pm
|
Junior Member
|
|
Join Date: Jan 30, 2018
Posts: 1
|
|
getting the fume not to over work.
I've gotten the fume to stick to my glass well. The problem i run in to after is trying to work my glass in to shape and still having the nice color of the gold or silver fume. instead i end up with a very dull milky white color is there any way to avoid this.
i've tried encasing the fume with a clear rod but even after that i'm left with a white dot.
This is happening to me mostly trying to get a nice fume color on implosion marbles and thick gathers.
I am using a bot cat gtt and boro glass fuming with .9999 silver on a quarts glass rod.
|
2018-01-31, 5:52am
|
|
hyperT
|
|
Join Date: Jan 31, 2013
Location: San Antonio, Texas
Posts: 582
|
|
Liquid Gold Tutorial
Save yourself some money. Just lightly coat a rod to use for fuming.
Download the tutorial.
|
2018-02-03, 7:20am
|
|
Marbles, dude, Marbles
|
|
Join Date: Jan 06, 2007
Location: Coral Springs, Florida
Posts: 653
|
|
Dull milky color usually means way too much silver. I did the Alien Skull marbles in the Boro Room. First I fumed
the Maria with a lot of gold for a few minutes to get a medium
to dark pink, and then just ONE or TWO passes of silver fume
to get green. Four or five passes of silver and I won’t get any green,
just a lot of white/grey.
__________________
A marble a day keeps the 'willies' away.
Gerald Kappel
To view links or images in signatures your post count must be 5 or greater. You currently have 0 posts.
|
Currently Active Users Viewing This Thread: 1 (0 members and 1 guests)
|
|
Posting Rules
|
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts
HTML code is Off
|
|
|
All times are GMT -7. The time now is 2:27am.
|